Pressure induced structural phase crossover of a GaSe epilayer grown under screw dislocation driven mode and its phase recovery | Scientific Reports

2D-GaSe has a honeycomb-like structure from the top-view, while a monolayer GaSe is composed of sandwiched links between two Ga atoms and two Se atoms along the side-view (Fig. 1a). For bulk GaSe, there are four different polytypes including β-(2H/D6h), ε-(2H’/D3h), γ-(3R/C3v), and δ-(4H/C6v), identified by AA’…, AB…, ABC…, and AA’B’B… stacking sequence of consecutive monolayers, respectively33. Experimentally, both ε-GaSe and γ-GaSe are generally co-existent in most of the epitaxial films and their bulk counterpart. In this work, high purity of 200 nm-thick single-crystalline 2D ε-GaSe thin films have been epitaxial deposited on GaAs (001) substrate by MBE for the high-pressure experiments. The growth conditions can be referred to our previous work22. As shown in Figs. 1b and S1a, the surface morphology of the epitaxial GaSe film grown under SDD growth mode typically exhibited in spiral-like structure. The samples were then mechanically polished to remove the GaAs substrate (Fig. 1c) and carved up to the appropriate sizes for loading into the DAC (Fig. 1d). Raman spectra of the GaSe film before and after substrate removal as shown in Fig. 1e confirm the success of the polishing process based on the elimination of the longitudinal-optical (LO) phonon at 291 cm−1 and transverse-optical (TO) phonon signal at 269 cm−1 of GaAs substrate. To confirm the dominant phase existing in the SDD film, Raman spectrum of the sub-free GaSe film were also carried out under 633 nm laser excitation. As can be seen in Fig. 1e, the emergence of the \({E}_{1g}^{2}\) Raman resonant mode (~ 251 cm−1) under 633 nm laser excitation that was unobservable under 532 nm excitation identifies the dominance of single ε-phase in the SDD-GaSe film22. Besides, no Raman peak shifting between the samples with and without substrate was observed, meaning that the localized strain potential generated at the film/substrate interface is negligible. High uniformity of the film quality was verified on a sizable area sub-free 2D ε-GaSe film (up to ~ 4 mm2) as revealed in Fig. S1b. This is also a valuable achievement of our work, offering flexible transferring to other substrates and scalable fabricating opto-electronic devices based on 2D-GaSe materials.

Anomalous out-of-plane incompressibility and structural transition in SDD-GaSe film

In order to verify the potential structural phase transition of the materials at high pressure, two parallel in-situ synchrotron ADXRD experiments were carried out on the 200 nm-thick free-standing ε-GaSe film and the GaSe bulk under hydrostatic pressurization at room temperature. The compressive pressure ranges for both samples were extended up to 35–40 GPa with fine increments of 0.5 GPa. Selected ADRXD patterns during compression are extracted from 2D-plate images (see Fig. 2a), where diffraction peaks of the SDD-ε-GaSe film are displayed (black arrows). As increasing the compression, all GaSe XRD peaks progressively shifted toward higher 2θ-angles along with broadening and diminishing in their linewidth and intensity, respectively. This is attributed to a gradual shrinkage of the crystal lattice with pressure. Indeed, refined d-spacing of the assigned diffraction planes of the GaSe film with pressure exhibits a compression as illustrated in Fig. 2b. As increasing the external pressure beyond ~ 20 GPa, foreign features located at 2θ angles of ~ 10.4°, ~ 14.8°, and ~ 20.9° started to be visible, while all hex-GaSe lines were continuously being suppressed and substantially disappeared at ~ 25 GPa. In comparison, the foreign features in the bulk appeared later than that in the GaSe film where its onset pressure is ~ 22 GPa (Fig. S2). The rise of alien diffractions is a signature of the structural phase transition from the hexagonal-to-rock salt (hex-to-RS) phase as reported previously29,34, where these XRD film peaks (blue arrows) can be assigned as (002), (220), and (004) diffraction lines of the GaSe rock-salt phase.

Figure 2figure 2

(a) Selected ADXRD spectra of the sub-free SDD-GaSe film during pressurization. (b) Refined d-spacing of the sub-free SDD-GaSe film as a function of applied pressure.

Full size image

To give a better understanding of the structural transition on the epitaxial film and bulk sample, we have analyzed the unit-cell volume (V) and the normalized cell parameters a(P)/a0, c(P)/c0, c(P)/a(P), and V(P)/V0 as a function of pressure, where a0, c0, and V0 are in-plane, out-of-plane lattice constant, and unit-cell volume at ambient conditions, respectively. Then, the individual lattice compressibility along a-axis and c-axis as well as the bulk modulus of the samples were quantitated using inverted Birch-Murnaghan Equation of State (BM-EoS) fitting as described in Eqs. (1–3)35,36:

$$\frac{a(P)}{{a}_{0}}={\left[1+\frac{{K}_{0a}^{^{\prime}}}{{K}_{0a}}P\right]}^{-\frac{1}{{K}_{0a}^{^{\prime}}}}$$

(1)

$$\frac{c(P)}{{c}_{0}}={\left[1+\frac{{K}_{0c}^{^{\prime}}}{{K}_{0c}}P\right]}^{-\frac{1}{{K}_{0c}^{^{\prime}}}}$$

(2)

and

$$\frac{V(P)}{{V}_{0}}={\left[1+\frac{{B}_{0}^{^{\prime}}}{{B}_{0}}P\right]}^{-\frac{1}{{B}_{0}^{^{\prime}}}}$$

(3)

where K0a (K0a) and K0c (K0c) are in turn in-plane (IP) and out-of-plane (OOP) inverse linear compressibility (its pressure derivative). Hereinafter K0a and K0c are called as IP and OOP incompressibility, respectively. B0 (B0) is the bulk modulus (its pressure derivative) of the materials.

The results are addressed in Fig. 3 and Table 1, including reproduced experimental data on GaSe bulk from U. Schwarz’s group for reference29. Figure 3a displays an excellent agreement in the pressure-dependent in-plane lattice constant (a) between our bulk sample and the referred study. Interestingly, even though the sub-free-SDD-GaSe film possesses a distinct layer-stacking configuration, i.e., spiral stacking, as compared to the layer-by-layer (LBL) stacking in bulk samples22, the pressure-dependent in-plane parameters observed in the GaSe film and the bulk samples are no visual difference. Indeed, the IP incompressibility values of these samples are comparable, which are ~ 186 ± 7 GPa (for sub-free SDD-GaSe film), 188 ± 7 GPa (GaSe bulk), and 198 ± 10 GPa (referred data). In other words, regardless of different layer stacking configurations, the in-plane compressibility in 2D-GaSe materials is identical. In contrast, the pressure-dependent out-of-plane lattice parameter of the SDD-GaSe film reveals an unusual phenomenon as shown in Fig. 3b,c.

Figure 3figure 3

(a–c) Pressure dependence of normalized lattice parameters of the sub-free SDD-GaSe film and GaSe bulk, in comparison to the reproduced data with permission from Ref.29. (d) Inverted Birch-Murnaghan EoS fitting of the sub-free SDD-GaSe film. (e) Unit-cell volume of the sub-free SDD-GaSe film as a function of pressure revealing a transition region (20–25 GPa) from hexagonal to high-pressure rock-salt phase.

Full size image

Table 1 Incompressibility parameter and bulk modulus of the SDD-GaSe film and GaSe bulk extracted from the inverted Birch-Murnaghan EoS.

Full size table

Its compression rate was nearly linear and much lower than that of the bulk samples, especially at the low-pressure range of < 5.0 GPa. In fact, from c(P)/c0 inverted BM-EoS fitting, while the OOP incompressibility of our GaSe bulk is in good agreement to the data of Schwarz et al.29, the K0c of SDD-GaSe film unveils a notable value of 164 ± 5 GPa, i.e., ~ 4 times higher in magnitude than those of the bulk samples. We claim that the classically spiral structure in SDD-GaSe film is much more incompressible and strongly close-packed along c-axis, which may be due to building up in coupling interaction between adjacent GaSe intra-layers, especially near SDCs. This behavior thus directly results in a ~ 1.7 times higher bulk modulus of the SDD-GaSe film (B0f. ~ 60 ± 4 GPa) as compared to that of the bulk sample (B0b ~ 35.5 ± 3 GPa) as noted in Figs. 3d and S3a. Furthermore, abrupt shrinkages in the unit-cell volume (V) that were observed at specific pressures, i.e., ~ 20 GPa for the SDD-GaSe film (Fig. 3e) and ~ 22 GPa for the GaSe bulk (Fig. S3b), are identified as the onset point of high-pressure GaSe RS phase29,34. It is noticed that the earlier RS onset point in the SDD-GaSe film could be subject to owning a large amount of SDCs in its unique crystalline structure and will be discussed later. Despite that, either the SDD-GaSe film or the GaSe bulk exhibits an equivalent end-point of the hex-to-RS structural phase transition (indicated by the completely quenching of GaSe XRD peaks) at ~ 25 GPa, which may be concurrent with the semiconducting-to-metallic electronic phase transition of the material28.

Optical phonon shifting under pressure in SDD-GaSe film

In-situ high-pressure Raman scattering measurement is also a powerful approach for gaining insight of the structural phase transition of the material via determining its phonon vibrational variation during compression31,37. Thus, this characterization was employed in this study on both samples. Due to the major ε-phase in the free-standing SDD-GaSe epitaxial film22, its crystal structure belongs to the non-centrosymmetric \({D}_{3h}^{1}\) group. Theoretically, it has 24 normal modes at the Γ point of the Brillouin zone, which is consisted of 11 non-degenerate Raman active modes, 6 non-degenerate IR active modes, and 2 acoustic vibration modes38,39. Figure 4a shows selected Raman spectra of the SDD-GaSe film during the experimental pressurization, where four typical phonon vibration modes of ε-GaSe, located at ~ 59.9 cm−1 (assigned to \({E}_{1g}^{1}\)); ~ 133.2 cm−1 (\({A}_{1g}^{1}\)); ~ 206.4 cm−1 (\({E}_{2g}^{2}\)), and ~ 308.3 cm−1 (\({A}_{1g}^{2}\)) have been observed at in-cell ambient pressure.

Figure 4figure 4

(a) Selected Raman spectra under 532 nm laser excitation of the sub-free SDD-GaSe film during pressurization. (b) Pressure dependence of phonon vibration modes observed from the sub-free SDD-GaSe film and the GaSe bulk. STP: standard temperature pressure at ambient. 532 nm excited Raman spectra of (c) the sub-free SDD-GaSe film and (d) the GaSe bulk before pressurization and after depressurization.

Full size image

As increasing the applied pressure, all of these modes (either IP or OOP vibration modes) gradually shifted towards the higher frequencies accompanied with their broadening in linewidth and deteriorating in intensity; and finally, were almost undetectable at ~ 29 GPa. It means that the layered structure of SDD-GaSe film was undergoing a great shortening not only in the vdW-interlayer gaps but also in the atomic distances in the intralayers, resulting in a visible lattice compression. Qualitatively, this behavior is well-consistent with what was observed from pressure-dependent ADXRD data presented above. To have a deeper insight, we plot the evolution of phonon vibration modes in the SDD-GaSe film and the bulk versus pressure as shown in Fig. 4b. The extracted pressure coefficient (defined by δ = dω/dP) and Grüineisen parameter of each Raman modes are also tabulated in Table 2.

Table 2 Experimental ambient-pressure frequency (ω0), pressure coefficient (δ), and Grüineisen parameter (

\(\overline{\gamma }\)

) of the Raman active modes observed from the SDD-GaSe film and the GaSe bulk.

Full size table

There are two noteworthy points from our analyses on SDD-GaSe film. Firstly, the \({E}_{2g}^{2}\) mode in the sub-free SDD-GaSe film at ambient pressure exposed an obvious redshift of 6.0 cm−1 as compared to that in the GaSe bulk. This corresponds to the unintentional appearance of both in-plane and out-of-plane strains induced by SDD-growth mode22,23. Even that, similar to the GaSe bulk, this vibration mode revealed a unity in pressure coefficient (δ ~ 2.4 cm−1/GPa) as the pressure increased up to ~ 16 GPa. This result is well-matched to the equivalency in IP incompressibility between SDD-GaSe film and GaSe bulk as extracted from the ADXRD data. Interestingly, above 16 GPa, the \({E}_{2g}^{2}\) frequency of SDD-GaSe film was getting close to that of GaSe bulk, and then those almost coincided with each other at pressures above 20 GPa. Thus, this tends to indicate a similar degree of compression in both SDD-GaSe film and GaSe bulk. Secondly, as observing the out-of-plane vibration modes of the SDD-GaSe film, i.e., \({A}_{2g}^{1}\) and \({A}_{2g}^{2}\) modes, their pressure-dependent behaviors could be noticed in two regions (Fig. 4b). In the first region (low-pressure range \(\le \) 5 GPa), both of these modes showed a lower blue-shifted rate than in the bulk’s one, corresponding to a smaller SDD-GaSe film’s δ value (Table 1). In other words, the lattice compression along c-axis at the low-pressure range is less pronounced in the SDD-GaSe film than in the bulk. Again, this statement is correlated to the high OOP incompressibility of the GaSe film (Fig. 3d). In the later region (> 5 GPa), the pressure coefficients of these modes in both GaSe film and bulk were approaching together since the lattice is less compressible when it is more and more close-packed.

It is necessary to take into account the simultaneous existence of ε– and γ-phase in the GaSe bulk grown by the Bridgman method40, as manifested by the appearance of extra broadband with centers located at ~ 235.1 cm−1 [\({A}_{1}(TO)\)] and ~ 251.4 cm−1 [could be a LO-mixed mode of \({A}_{1}(LO)\) at ~ 247 cm−1 and \({E}_{1g}^{2}(LO)\) at ~ 253 cm−1] in Raman spectrum of the GaSe bulk at ambient pressure (Fig. S4)39. As increasing the applied pressure, the LO-mixed mode monotonously shifted to the higher frequencies with a smaller pressure coefficient δ as compared to that of \({E}_{2g}^{2}(TO)\), then is almost undetectable at ~ 16 GPa. On the other hand, the \({A}_{1}(TO)\) peak, which is considered as a signature of γ-GaSe39,41, exhibited an abnormal trend upon compression by nonlinearly shifting to the lower frequencies in a wide range of pressure up to ~ 25 GPa, and then disappeared at the end-point of the hex-to-RS phase transition. The observed negative pressure coefficient of the \(\gamma -{A}_{1}(TO)\) mode could be explained well when the competition between interlayer interaction and Ga-Se chemical bond-tilting effect along with the atomic vibration direction of three observed OOP modes (Fig. S4b) are taken into consideration. For the \({A}_{1g}^{1}\) mode, two Se atoms in an intralayer vibrate out-of-phase to each other, whereas Ga and Se atom vibrations are in-phase. Thus, this mode is only governed by the strong interlayer interaction since the bond-tilting effect is negligible, showing a high positive δ (see bold values in Table 2). Different from \({A}_{1g}^{1}\) mode, these effects are visible (out-of-phase vibration presented in either Se/Se or Ga/Se pair) and compensate each other in the \({A}_{1g}^{2}\) mode, leading to a smaller positive δ. On the contrary, the interlayer interaction could be ignored in the \(\gamma -{A}_{1}(TO)\) mode due to the in-phase vibration between Se atoms in each intralayer as well as interlayer, while the Ga/Se out-of-phase vibration could strongly promote the bond-tilting effect, resulting in the negative δ of this mode. Moreover, the pressure-induced redshift phonon frequency could be a characteristic of the TO-LO splitting due to the long-range Coulomb interaction. This behavior was also observed in some Se-based 3D-conventional semiconductors such as ZnSe, ZnFeSe, and ZnMnSe42,43.

Unique structural phase reversibility in SDD-GaSe film

After compressing the material up to ~ 35 to 40 GPa, the samples were gradually decompressed back to ambient pressure. The down-stroke Raman spectra of both SDD-GaSe and the bulk samples are shown in Fig. S5. In the case of SDD-GaSe film, it seems likely that the non-polar out-of-plane vibration mode-\({A}_{1g}^{1}\) was revived at the very early stage of the depressurization, then gradually redshifts, and being pronounced at ~ 4.8 GPa along with the appearance of the signal from in-plane vibration mode (\({E}_{2g}^{2}\)). On the other hand, the down-stroke spectra starting from 30 GPa of the bulk sample revealed the gentle revitalization of a broadband relating to \({A}_{1g}^{1}\) and \({A}_{1}(TO)\) modes. Interestingly, after completely releasing external pressure, the Raman spectrum of SDD-GaSe film exhibited a reversible property, where all SDD-GaSe Raman active modes were well-recovered (Fig. 4c). The enhancement of a broad-peak located at ~ 155 cm−1 may be due to the laser-induced oxidation after the long time-experiment. Besides, the slight redshifts of all Raman features are attributed to the distorted lattice structure after compression. On the contrary, the decompressed Raman spectrum of bulk-GaSe is irreversible with the dominance of γ-phase signal at the end (Fig. 4d). These results might be due to the differences in the high-pressure structural phase transition mechanism between the Bridgman-grown GaSe bulk and the MBE-grown SDD-GaSe film. We claim that the bulk sample may undergo the layer-sliding process upon compression, while the SDCs play a major factor in promoting the phase transition in SDD-GaSe under high pressure.

Role of screw dislocation cores

Previous researches have shown that because of the typical LBL-vdW structure of most 2D materials, they have possibly experienced the layer sliding under high pressure44,45. In agreement with our experimental findings as shown in the ADXRD data, the slope changing (from negative to positive) in the GaSe bulk c/a profile (Fig. 3c) at ~ 16 GPa is said to be evidence of pressure-induced layer sliding, leading to the alteration in the layer-stacking configuration. As looking back on Fig. 1a, the difference in stacking configuration between γ and ε-GaSe phase is only the horizontal translation of the third rigid-layer (noted by layer C). Thus, it is a possible occurrence of ε-to-γ phase transition due to the layer-sliding effect during pressurization. Indeed, in the LBL-GaSe bulk sample, the LO-mixed mode almost disappeared at ~ 16 GPa, whereas the \({A}_{1}(TO)\) mode that belonged to γ-phase could survive up to ~ 25 GPa (Figs. 4b and S4a). This means that the high-pressure (HP) phase transition in the case of LBL-GaSe bulk could include a ε-to-γ phase transition, followed by the hex-to-RS structural transition. In light of these observations, we suppose that the pressure-induced ε-to-γ phase transition via the layer-sliding phenomenon in the LBL-GaSe bulk required a large amount of activation energy, which could be the main reason for the phase irreversibility of the LBL-GaSe bulk after decompression as mentioned above. On the other hand, the MBE-grown SDD-GaSe film is supposed to undergo a distinctive pressure-induced structural phase transition mechanism, where the SDCs play a major driving force in the hex-to-RS transformation and vice versa. To describe visibly the scenario, we make a high-pressure structural phase transition diagram of SDD-GaSe as shown in Fig. 5. Firstly, our previous study has demonstrated that the growth of SDD-GaSe is hypothesized to experience an edge climb-up process at SDCs, where the Se-Se inter-edge dimerization was taking place (Fig. S6), resulting in the discontinuity in the atomic chain-layer, and hence, enhancing the interlayer interaction46. As a result, the SDD-GaSe film is more incompressible along the c-axis than that of the LBL-GaSe bulk presented by the four-times larger in the OOP incompressibility and lower pressure coefficient δ of SDD-GaSe. Furthermore, according to the climb-up mechanism in the SDD-GaSe film, it is acceptable to assume that the intralayer Ga-Ga bonds located near the SDCs are mostly unstable. Secondly, at sufficient applied pressure, the pressure-induced intralayer-to-interlayer charge transfer becomes dominant, leading to further weakening of the Ga-Ga bonding strength47. Thus, the SDCs could play as the primers to initiate disruption of the neighbored Ga-Ga covalent-bonding chains, followed by the rearrangement of free half-rigid layers. Finally, the Ga and Se atoms from adjacent half-rigid layers catch each other to form Ga-Se metallic bonds, which is similar to the bonds in the GaSe RS structure. Although the SDD-GaSe film is more incompressible, it seems to be more brittle as compared to the GaSe bulk because of possessing an intensely high-density of SDCs in its lattice structure. The HP phase transition barrier in SDD-GaSe could be smaller than that of the LBL-GaSe structure. In other words, SDCs could assist the hex-to-RS transition to occur earlier, evidenced from the lower RS onset point of SDD-GaSe film compare to that of the bulk. However, it is possible that the SDCs were still being memorized in the RS structure of the SDD-GaSe film because of the strong coupling between adjacent haft-rigid layers near the SDC sites. Therefore, as entirely releasing the sample from the external pressure, these SDCs could now promote the recovery of the original layer-stacking configuration as observed from the well-recuperated ε-GaSe Raman modes.

Figure 5

figure 5

A summarized evolution of the structural phase transition occurring in a free-standing SDD-GaSe film under external pressure.